常用塑胶模具收缩率一览表
编制单位:技质科 编制:唐成保
序 玻璃纤维
密度
收缩率
号
缩写代码
树脂全称
含量
(g/cm)
%
1
ABS
AcrylonitriteButadiene Styrene
/
1.05
0.5%
2
ABS+10%GF
AcrylonitriteButadiene Styrene+10% Glass Fiber
10%GF
1.16
0.4%
3
ABS+20%GF
AcrylonitriteButadiene Styrene+20% Glass Fiber
20%GF
1.24
0.3%
4
ABS+30%GF
AcrylonitriteButadiene Styrene+20% Glass Fiber
30%GF
1.31
0.3%
5
PC
Polycarbonate
/
1.20
0.6%
6
PC+10%GF
Polycarbonate+10% Glass Fiber
10%GF
1.26
0.5%
PC+20%GF
Polycarbonate+20% Glass Fiber
20%GF
1.27
0.4%
PC+30%GF
Polycarbonate+30% Glass Fiber
30%GF
1.30
0.3%
PC+ABS
Polycarbonate+AcrylonitriteButadiene Styrene
/
1.15
0.5%
AS
Acrylonitrite Styrene
/
1.07
0.6%
PMMA
Polymethyl Methacrylate(Acrylic)
/
1.18
0.4%
POM
Polyacetel
/
1.42
2%
PA66
Polyamide-66
/
1.16
1.3%
PA66+10%GF
Polyamide-66+10% Glass Fiber
10%GF
1.4
0.6%
PA66+20%GF
Polyamide-66+20% Glass Fiber
20%GF
1.41
0.5%
PA66+30% GF
Polyamide-66+30% Glass Fiber
30%GF
1.52
0.45%
PA6
Polyamide-6
/
1.15
0.8%
PBT
Poly(Butylene Terephthalate)
/
1.38
1.5%
PBT+10% GF
Poly(Butylene Terephthalate)+10% Glass Fiber
10%GF
1.60
0.7%
PBT+20% GF
Poly(Butylene Terephthalate)+20% Glass Fiber
20%GF
1.60
0.6%
PBT+30% GF
Poly(Butylene Terephthalate)+30% Glass Fiber
30%GF
1.66
0.5%
PP
Polypropylene
/
0.91
1.5%
耐高温PP
High Heat Polypropylene
/
1.12
1.0%
PP 防火
Flame Retarded Polypropylene
/
0.95
1.4%
软氯PVC
Polyvinyl Chloride Plasticized
/
1.35
1.5%
低密 LDPE
Low Density Polyethylene
/
0.93
2%
高密HDPE
High Density Polyethylene
/
0.98
3%
弹性体TPE
Polyester Thermoplastic Elastomer
/
0.92
1.5%
PPS
Polyphenylene Sulfide
/
1.67
0.25%
LCP
Liquid Crystal Polymer
/
1.70
0.02%
TPU
Thermplastic Polyurethane
/
1.24
1.2%
备注:1)收缩率会受加工条件及模具设计的影响而改变;
取向不同,在垂直于流动方向的收缩可能较小(流动方向收缩为横向的 1.6 倍;对于结晶性树脂的倍数更大);
确定的模具及产品设计,最先制作样模,以得到更准确的收缩值;